The Properties of A-PET sheet (Normal Grade)
|
Properties |
A-PET sheet (Normal Grade) |
|
|
|
Typical Value |
Unit |
|
Density |
1.34 |
g/cm 2 |
|
Thickness |
250 - 500 + 10 |
microns |
|
Thermal |
|
|
|
Glass temperature DTA |
68-77 |
C |
|
Glass transition temperature |
86 |
C |
|
Melting range |
255 |
C |
|
Vicat softening temperature, VST/B/120 |
73 |
C |
|
Heat deflection temperature |
70 |
C |
|
Method A |
72 |
C |
|
Method B |
80x10-6 |
K-1 |
|
Coefficient of linear expansion |
1.3 |
kJ/kg K |
|
Specific heat capacity |
0.24 |
W/m K |
|
Thermal conductivity |
|
|
|
Electrical |
|
|
|
Surface resistance |
5x1012 |
ohm |
|
Volume resistivity |
2x1012 |
ohm.cm |
|
Dielectric constant 50 Hz |
3.6 |
- |
|
1 Mhz |
3.4 |
- |
|
Dissipation factor 50 Hz |
0.002 |
- |
|
1 Mhz |
0.030 |
- |
|
Dielectric strength |
45 |
kV/mm |
|
Mechanical |
|
|
|
Tensile strength @ Yield |
|
|
|
MD |
55 |
N/mm2 |
|
TD |
55 |
N/mm2 |
|
Tensile strength @ Break |
|
|
|
MD |
42 |
N/mm2 |
|
TD |
38 |
N/mm2 |
|
Elongation @ Yield |
|
|
|
MD |
3.5 |
% |
|
TD |
3.5 |
% |
|
Elongation @ Break |
|
|
|
MD |
300 |
% |
|
TD |
300 |
% |
|
Tensile Modulus of Elasticity |
|
|
|
MD |
2,200 |
N/mm2 |
|
TD |
2,200 |
N/mm2 |
* Typical Values represent an average of samples tested using ASTM standard proceduces. They are provided as general information only and are not part of product specification.